Sandwich Corrosion per ASTM F 1110 Page
SMI Inc.
SCIENTIFIC MATERIAL INTERNATIONAL
12219 SW 131 Avenue Miami, Florida 33186-6401 USA
Phone (305)971-7047 Facsimile (305) 971-7048
Attn: Larry Holt Date: 28-Aug-1995
Holt International LLC
1060 Yaple Rd. SMI/REF: 9508002-R
Kingston, OH 45644 Reissued for name change only.
Product: E-Z Grip (Marine Formula) (rec'd 16-Aug-1995)
Dilution: As received (shaken well before testing)
Sandwich Corrosion
per ASTM F 1110
TEST METHOD
- Aluminum panels having clad or anodized nonclad surfaces are sandwiched together with filter paper saturated with the test material between the panels. The sandwiched panels are cycled between warm ambient air and warm humid air for 7 days. The coupons are then inspected to determine whether corrosion more severe than that caused by a reagent water has occurred on the surfaces exposed to the test material. This test method may be used for solutions of dry granular material or for liquid materials.
- Relative corrosion severity rating system:
- No visible corrosion
- Very slight corrosion or discoloration (up to 5% of surface area corroded)
- Slight corrosion (5 to 15%)
- Moderate corrosion (10 to 25%)
- Extensive corrosion or pitting (25% or more)
| |
2024-T3 Bare Anodized |
2024-T3 Alclad |
7075-T6 Bare Anodized |
7075-T6 Alclad |
As received |
1 |
1 |
1 |
1 |
CONTROL |
1 |
1 |
1 |
1 |
Result: Conforms
Respectfully submitted,