Hydrogen Embrittlement per ASTM F 519, Type 1C Page
SMI Inc.
SCIENTIFIC MATERIAL INTERNATIONAL
12219 SW 131 Avenue Miami, Florida 33186-6401 USA
Phone (305)971-7047 Facsimile (305) 971-7048
Attn: Larry Holt Date: 11-Apr-1995
Holt International LLC
1060 Yaple Rd. SMI/REF: 9503083-R
Kingston, OH 45644 Reissued for name change only.
Product: E-Z Grip FRICTION DROPS
Dilution: As received
Hydrogen Embrittlement
per ASTM F 519, Type 1C
Test Procedure:
- TYPE 1C SPECIMENS
- Load a minimum of three specimens to 45% of the bend strength.
- Put the test solution into a clean plastic container, place the stressed specimens in the test solution, and record the time to failure if less than 150 hours. The test may be discontinued after 150 hours.
INTERPRETATION OF RESULTS
- Failure of all specimen types occurs by readily visible detectable fracture processes.
As received: No failures within 150 hours. (Product layers upon standing)
Result: Conforms
Respectfully submitted,
Patricia D. Otero, SMI Inc.
|